What lost-wax casting is, in one paragraph
You make a wax copy of the part, build a ceramic shell around it, melt the wax out, fill the empty cavity with liquid metal, and break the shell off. That is the whole process. Everything difficult about it comes from the second half of that sentence: the shell has to survive a thermal shock of several hundred degrees, the metal has to reach the last corner of the cavity before it freezes, and neither of those things leaves much room for error.
Lost-wax casting — investment casting, cire perdue, precision casting, the names are interchangeable in practice — sits at CT4 to CT7 on the dimensional scale, which is why it gets used for parts that arrive at the machine shop with 1 mm of stock instead of 4 mm. The trade-off is cost per kilogram. Below roughly 0.1 kg the process is hard to beat. Above 20 kg the shell cost and the handling risk start pushing you back toward sand.
Where it sits against the alternatives
Most sourcing arguments about lost-wax casting are really arguments about tooling amortisation. The table is the one we use in quotation conversations.
| Process | Typical tolerance | Tooling | Economic batch | Wall thickness floor |
|---|---|---|---|---|
| Lost-wax (silica sol shell) | CT4–CT6 | Aluminium wax die, 4–8 weeks | 200 – 50,000 pcs/yr | 1.5 mm (steel), 1.0 mm (aluminium) |
| Lost-wax (water glass shell) | CT6–CT7 | Aluminium wax die | 500 – 100,000 pcs/yr | 2.0 mm |
| Green sand | CT8–CT12 | Pattern only | 1 – 500 pcs | 4 mm |
| High-pressure die casting | CT4–CT7 | Hardened steel die, 10–16 weeks | 10,000+ pcs/yr | 0.8 mm, but porosity limits pressure-tightness |
| Sand casting + machining | CT8–CT12 | Pattern only | 1 – 1,000 pcs | 5 mm |
The number people forget is the tooling lead time. A wax die is not a cheap pattern; it is a machined cavity that has to release a fragile wax pattern without dragging it. Four to eight weeks is normal, and any supplier quoting two weeks is either cutting the die or planning to hand-finish every wax.
The eight steps that decide whether you get good parts
Each step below carries the parameter range we work to. Treat these as ballpark figures for a steel foundry on silica sol shells — your supplier’s card governs, and the differences between foundries on the same step are larger than the differences between the published ranges.
1. Wax injection
Wax at 54 ± 2 °C, injected at 4.2 MPa, held 5–15 s depending on section. The failure mode here is not a bad-looking pattern; it is a pattern that looks fine and has a shrink void under a thick boss. That void becomes a ceramic core in reverse — the shell fills it, the metal cannot, and you get a porosity report six weeks later. Wax that has been held hot too long also loses its ability to fill thin sections, which shows up as short shots on 1 mm ribs and nowhere else.
2. Cluster assembly
Patterns are glued to a central sprue, usually at an angle rather than flat, so the metal enters the cavity without a free fall. This is the step where most shops cut corners to fit more parts per cluster. More parts per cluster lowers cost per piece and raises the chance that the first parts to fill are starved of feed metal. A cluster that runs 60 pieces usually produces a narrower process window than one that runs 40.
3. Shell building
Four and a half coats for small parts; eight and a half for high-precision work with tight dimensional control. Face coat slurry is fine zircon or fused silica; backup coats are coarser mullite or chamotte. The humidity numbers matter more than the coat count:
- Face coats: 60–70% RH, no forced air movement. Dry too fast and the binder skins over while the interior is still wet, which cracks the coat from the inside.
- Backup coats: 40–60% RH with 6–8 m/s air. This is where you want evaporation.
Layer-by-layer drying failures rarely show as shell cracks. They show as a rough casting surface, because the delaminated layer lifts during pour and the metal fills the gap.
4. Dewaxing
Steam autoclave, 0.6–0.75 MPa, pressure raised over 2–3 min. Raise it faster and the wax boils inside the shell before it can flow out through the gate; the resulting internal pressure is what puts hairline cracks in the shell that nobody sees until the casting leaks. This is the single most underestimated step in the process. A shell that survives dewaxing with a 0.2 mm crack will pass every visual check and fail a pressure test.
5. Firing
1150–1195 °C in an oil-fired kiln, 1125–1175 °C in an electric one, held long enough that the shell comes out white or rose-coloured. Any residual carbon from the wax burns out here. Come out early and the carbon stays in the face coat, which shows up as gas porosity clustered on the surface of the casting, right where the shell touched it.
6. Melting
For stainless and low-alloy steel in a medium-frequency induction furnace: charge, melt to 1550 °C, pre-deoxidise, refine at 1580–1600 °C, then final deoxidation with pure aluminium immediately before tapping. The aluminium addition is where inexperienced crews cause brittle fracture — too much, and you get alumina stringers and low impact toughness; too little, and the oxygen stays in the bath and reports as porosity. If deoxidation has been sloppy, the fracture surface of a test bar will show a grey, crystalline appearance instead of a ductile cup-and-cone.
7. Pouring
Shell temperature 700–850 °C, and no more than 10 s between pulling the shell from the kiln and the metal hitting the sprue. Every second of that gap is heat leaving the shell and the metal getting one step closer to freezing before it reaches the thin sections. The pouring rate is the other half of the problem: fill too slowly and the metal front stalls and oxidises; fill too fast and you entrain air and mould gas that cannot escape through the shell fast enough.
8. Knockout, cut-off, finishing
Shell removal by vibration, gate removal by abrasive cut-off, then grinding, heat treatment, NDT. This is also where you find out whether steps 1–7 were right, because the defects generated upstream are all sitting in the parts by now and none of them can be fixed by finishing.
Design rules that prevent most of the defects
A drawing that respects five rules will cast well at almost any competent foundry. A drawing that violates them will produce arguments at every foundry you send it to.
- Uniform wall. Keep sections within a 2:1 ratio. The metal always feeds the thin section from the thick one, and a 4:1 ratio means the thick section is a shrink cavity waiting to happen.
- Fillets, not sharp corners. Minimum internal radius 1 mm, ideally 1.5 mm or 0.5× wall thickness. Sharp corners are hot spots, and hot spots are where the last liquid metal sits and shrinks.
- Draft on every vertical face. 1–2° is enough for a machined wax die, but it has to be there. Zero draft means every wax pattern is hand-pried out, and the rejection rate on hand-pried patterns is not the foundry’s fault.
- Holes cast, not drilled, up to 6× diameter depth. Beyond that the ceramic core that forms the hole starts to bend under the metal’s buoyancy. A 3 mm hole at 20 mm depth casts reliably; at 30 mm it does not.
- No isolated thin fins. Anything under 1.2 mm attached to a 6 mm body will be cold shut unless the foundry preheats the shell at the top of its range and pours hot — which then costs you on the thick section.
The five failure modes you will actually see
In order of how often they appear in a rejection report, with the mechanism behind each one.
Shrinkage porosity
Open or closed cavities at the thermal centre of a thick section, with a rough dendritic interior. The metal froze before feed metal could replace the volume lost to contraction. Fix by adding a riser with modulus at least 1.2× the casting’s, or by changing the section so it does not need feeding at all. The second option is almost always cheaper.
Hot tearing
Intergranular cracks, usually at a junction where a thin section meets a thick one, found after knockout rather than before. The metal is tied between a thick region that is still contracting and a thin region that has already become rigid. More fillet, less restraint, or a different gate position.
Gas porosity
Smooth-walled, round, often clustered near a surface or at the top of the casting. Two sources: hydrogen from a wet charge or a damp shell, and air entrained during filling. If the voids are near the gate, it is entrainment; if they are distributed through the section, it is gas in solution. The distinction matters because the fixes have nothing to do with each other.
Inclusions and sand inclusions
Irregular, angular, often with a dark rim. Either refractory from the shell face — a sign of a weak face coat or a pouring temperature that attacked it — or oxide from a turbulent fill. Both are eliminated by the same class of changes: calmer filling and a stronger face coat.
Dimensional drift
Not a defect in the metallurgical sense, but the most expensive one in the machine shop. Wax shrinks, metal shrinks, and the shell expands during firing. A die cut to nominal will not produce a nominal part. The compensation is foundry-specific and has to be built into the die from measured data, not from a handbook coefficient.
Alloys, and the ones that behave differently
Carbon and low-alloy steel, stainless (CF8, CF8M, CF3M, CA15, CA6NM), nickel-base superalloys, cobalt alloys, aluminium and copper alloys all run the same process with different pouring temperatures and different shell chemistry.
The trap is substitution. CF8M and CF3M look interchangeable on a drawing and are not — the carbon difference changes weldability and intergranular corrosion resistance. Replacing a wrought 316 part with a CF8M casting changes the mechanical properties in ways that a simple strength check will not reveal. We keep a longer comparison of grades across five national standards, and a separate write-up on which substitutions are safe.
Tolerances and surface finish you can actually get
A general tolerance of ±0.1 mm on the first 25 mm and ±0.02 mm per 25 mm beyond that is a reasonable commercial expectation on a silica sol shell in a stable shop. Ra 3.2–6.3 µm on as-cast surfaces. Anything tighter is either selectively ground or it is a promise that will not hold across a production run.
The tolerance table by dimension band, and the surface finish you should expect per alloy, are on the data sheet page.
What to send for a quotation
Three things, in this order: a 3D model (STEP preferred, IGES acceptable), a 2D drawing with the critical dimensions and tolerances marked, and the annual quantity plus the expected batch size. The last one changes the answer more than people expect, because it decides whether the wax die is built for 5,000 shots or 50,000.
If the part has a pressure-tightness requirement, say so at quotation stage. It changes the gating design, the NDT plan, and sometimes the alloy.
We put the arithmetic for piece weight, yield and cost stack on the tools page, including the alloy addition calculation for the melt.
Questions we get asked most
How small can a lost-wax casting be?
A few grams. Below about 5 g the handling of the wax pattern becomes the limiting factor rather than the casting itself, and the cost per piece stops falling with size.
Can lost-wax casting hold a pressure-tight part?
Yes, with the right gating and a shell that did not crack during dewaxing. Pressure tightness is a process-discipline outcome, not an alloy property. If a supplier cannot tell you their dewaxing pressure ramp, ask again.
What is the minimum order quantity?
It is set by the wax die, not by the process. Once the die exists, 50 pieces and 5,000 pieces run through the same line. The real question is whether the die cost amortises over your volume.
How long does a first article take?
Six to ten weeks for a new die plus first-article samples, assuming the drawing is final. Die changes after first article are where schedules actually slip.
Does the process work for aluminium?
Yes, and it is common for thin-wall aluminium housings. The pouring temperature is lower, the shell chemistry is gentler, and the tolerance is usually better than steel because the thermal contraction is more uniform.
Further reading
- Material selection and cross-standard grade comparison — how to pick an alloy before you pick a foundry.
- Process calculators — piece weight, yield, cost stack, ferroalloy additions, riser modulus.
- Dimensional and material data sheet — tolerance bands, surface finish, mechanical properties.
- Casting defect reference — symptom, mechanism and correction for the common failure modes.
- All articles — shell building, slurry control, dewaxing and firing in more depth.